Skip to content
SubmittalForge

CSI 22 11 00 / 33 11 00 — Facility & Utility Water Piping

ASTM A53 Grade B mill test report checklist

Standard Specification for Pipe, Steel, Black and Hot-Dipped, Zinc-Coated, Welded and Seamless

Chemistry (% by weight)

Carbon (C)
≤ 0.3%
Manganese (Mn)
≤ 1.2%
Phosphorus (P)
≤ 0.05%
Sulfur (S)
≤ 0.045%
Copper (Cu)
≤ 0.4%
Nickel (Ni)
≤ 0.4%
Chromium (Cr)
≤ 0.4%
Molybdenum (Mo)
≤ 0.15%
Vanadium (V)
≤ 0.08%

Tensile requirements

Yield strength
≥ 35 ksi
Tensile strength
≥ 60 ksi
Elongation in 2 in.
≥ 29.5%

Build America, Buy America

2 CFR 184.3

On federally funded infrastructure, ASTM A53 Grade B material is an iron or steel product: every process from initial melting through coating must happen in the United States. The mill test report should show a U.S. melt and pour location for each heat.

Edition, notes and sources

Checked against A53/A53M-24 (Types S and E)
  • Minimum elongation in 2 in. is e = 625,000·A^0.2 / U^0.9 (A = specimen area, capped at 0.75 in²; U = 60,000 psi). 29.5% is the value at A = 0.75 in²; smaller specimens require less, so a shortfall is flagged for review, not failed.
  • The five elements Cu, Ni, Cr, Mo and V combined may not exceed 1.00%.

Sources

ASTM standards are copyrighted. These limits were cross-checked against published summaries; confirm them against a licensed copy of the edition your specification cites.

Reviewing an ASTM A53 Grade B mill test report

  • Confirm the MTR names ASTM A53 Grade B (or a dual certification that includes it).
  • Match the heat number on the MTR to the heat stamped on each delivered piece.
  • Compare the heat analysis with the chemistry limits above.
  • Compare the tensile results with the yield, tensile and elongation minimums.
  • On BABA work, confirm the country of melt and pour is the United States.